Welding Inspection

Destructive vs Non-Destructive Weld Testing: Which Tests a PQR Needs and Which Tests Production Welds Need

Thermite weld mold clamped on a rail with two preheating flames rising from it, on ballasted track with concrete ties, the kind of rail weld whose procedure is qualified by destructive tests before it is used in track
Photo: St Gallen - Track Welding (31595736235) by Kecko, CC BY 2.0, via Wikimedia Commons.

Destructive weld testing breaks specimens cut from a test weld to prove that a welding procedure or a welder can produce sound metal; non-destructive testing examines the welds that stay in the structure. A groove-weld procedure qualification record (PQR) under AWS D1.1 or ASME Section IX is commonly reported as two tension and four bend specimens.

A note on sources. AWS D1.1, ASME Section IX, API 1104, AWS D15.2 and the AREMA manual are paywalled. Specimen counts, acceptance limits and D1.1:2025 clause numbers below come from study references and technical articles that agree with one another. Confirm each against the edition your contract names. Federal rules are quoted from the regulation text.

What is the difference between destructive weld testing and non-destructive testing?

Destructive weld testing answers "can this procedure, or this welder, make a sound weld with the required properties?" Non-destructive testing (NDT) answers "is this particular weld acceptable?" The first is done once, on a test coupon that is cut up. The second is done on welds that must still carry load afterward.

Federal pipeline safety rules state the split in two sentences. For gas pipelines, 49 CFR 192.225 says:

"The quality of the test welds used to qualify welding procedures must be determined by destructive testing in accordance with the applicable welding standard(s)."

For the welds that go into the ground, 49 CFR 192.243 says:

"Nondestructive testing of welds must be performed by any process, other than trepanning, that will clearly indicate defects that may affect the integrity of the weld."

Trepanning cuts a plug out of the weld, so the rule excludes the one sampling method that damages the production weld. Structural, pressure and rail codes follow the same logic.

Destructive testingNon-destructive testing
Question answeredCan the procedure or the welder produce the required strength, ductility, soundness and toughness?Does this weld meet the acceptance criteria?
What is testedSpecimens cut from a test plate, test pipe or sample rail weldThe production weld itself
What happens to the weldIt is pulled, bent, broken, sectioned or indentedIt stays in service
WhenBefore production, and again when an essential variable changesDuring and after production, at the extent the code or contract sets
Properties measuredTensile strength, ductility, hardness, impact energy, fusion on a cut or broken faceNone directly; it detects and sizes discontinuities
Typical recordPQR or welder qualification recordVisual, UT, RT, MT or PT report
Who does itThe qualifying organization, usually through a mechanical testing laboratoryInspectors and NDT personnel

Key takeaway: a passed PQR says the procedure works; it says nothing about weld number 47 on the job, and a clean ultrasonic report on weld 47 says nothing about its tensile strength.

Which destructive tests does a PQR need?

A groove-weld PQR is built on tension tests and guided bend tests, with macroetch for fillet and partial-penetration procedures and Charpy impact tests only where toughness is specified. The count and type of specimen come from the code that governs the work.

Code and weldDestructive tests on the test weld (as reported in public sources)Non-destructive tests on the test weld
AWS D1.1, CJP groove weld on plate2 reduced-section tension specimens; 4 bend specimens (2 root and 2 face at 3/8 in. and thinner, 4 side bends above that); Charpy V-notch only when the contract documents specify itVisual inspection of the whole test plate, then RT or UT, before specimens are cut
AWS D1.1, fillet weldMacroetch specimens from a T-test, plus a consumables verification testVisual inspection
ASME Section IX, groove weldTension tests (QW-150) and guided bend tests (QW-160), commonly 2 and 4; toughness tests (QW-170) when the construction code requires them; fillet-weld tests (QW-180) for fillet proceduresNone listed on the suggested PQR form
API 1104, pipeline girth weldNick-break specimens, with tension and bend specimens, cut from the test jointNot the basis of procedure qualification under 49 CFR 192.225 and 195.214
AWS D15.2, thermite or flash-butt rail weldSlow bend, hardness and, by weld type, chemistry or macroetch (titles of Tables 6.4, 6.6 to 6.8 and Figures 6.1 to 6.4)Clause 8 covers visual and ultrasonic inspection

D1.1 screens the test plate with NDT first. A study reference for the 2025 edition lists the tests for a complete-joint-penetration (CJP) qualification as visual inspection, NDT of the completed coupon, bend tests and tension tests (clause 6.11.3, with specimen types by thickness in Table 6.2). A plate that fails radiography or ultrasonic testing isn't worth machining.

ASME Section IX records mechanical tests only. ASME's suggested PQR format, Form QW-483, has blocks for "Tensile Test (QW-150)", "Guided-Bend Tests (QW-160)", "Toughness Tests (QW-170)" and "Fillet-Weld Test (QW-180)", plus "Other Tests". The form has no block for radiography or ultrasonic results. Section IX has no prequalified procedures, so every ASME procedure goes through these tests.

A prequalified D1.1 procedure needs none of them. A WPS written inside every Clause 5 limit is exempt from qualification testing, which is why many structural shops never break a specimen. Our WPS vs PQR guide covers the two routes and the thickness ranges a PQR qualifies; this article covers the tests themselves.

Key takeaway: ask which code governs before asking which tests are needed, because the same 1 in. plate is tested differently under D1.1, Section IX and API 1104.

What does each destructive test prove?

Each destructive test isolates one property: the tension test measures strength, the bend test exposes unsoundness and low ductility, the macroetch shows fusion and penetration, break tests show the inside of the weld, hardness flags brittle zones and the Charpy test measures notch toughness.

Tension test

A reduced-section specimen is cut across the weld, the reinforcement is machined flush and the specimen is pulled until it breaks. Tensile strength is the maximum load divided by the original cross-sectional area (TWI, tensile testing). Study material for D1.1 gives the acceptance rule as a tensile strength not less than the minimum specified for the base metal, and a break in the base metal at or above that value passes. The test proves joint strength, not freedom from small flaws: a ductile joint can carry the load around them.

Guided bend test

A strip cut across the weld is bent around a former so that the root, the face or the side of the weld is stretched. TWI describes what that does:

"The outside of the bend is extensively plastically deformed so that any defects in, or embrittlement of, the material will be revealed by the premature failure of the coupon." (TWI, bend testing)

The scope of ASTM E190, the guided bend test method for welds, adds a point that matters for this comparison: "Flaws, not shown by X rays, can appear in the surface of a specimen when it is subjected to progressive localized overstressing." A bend test can therefore fail a coupon that passed radiography. Study material for D1.1 reports the acceptance limits as no single opening over 1/8 in. on the convex surface and a 3/8 in. limit on the sum of smaller openings, with corner cracks treated separately. TWI gives the general rule that most specifications reject a defect over 3 mm.

Macroetch test

A cross-section is cut, polished and etched so the weld passes, fusion boundary and heat-affected zone show. It is the main test for fillet and partial-penetration procedures, where the questions are whether the weld fused to the root and whether the size is there. ASME's PQR form records it under the fillet-weld test with a "Penetration into Parent Metal" entry and a line for the macro results.

Nick-break and fillet break tests

Both break the weld open so the inspector reads a fracture face. In a nick-break test the specimen is notched so that it fractures through the weld metal, exposing porosity, slag and lack of fusion; it is associated with API 1104 pipeline qualification. In a fillet break test a one-sided T-joint is folded over until the fillet breaks or bends flat. Neither test gives a strength number.

Hardness test

An indenter is pressed into a prepared surface and the size of the impression gives the hardness. Brinell tests use a ball (10 mm under 3,000 kgf for steel) and average over a wide area. For a survey across a weld, TWI notes that the Brinell test "cannot be used to determine the hardness variations in a welded joint for which the Vickers test is preferred" (TWI, hardness testing). High heat-affected-zone hardness warns of a brittle structure.

Charpy V-notch impact test

A notched bar is broken by a pendulum at a set temperature and the absorbed energy is recorded. The standard specimen is "55mm long, 10mm square and has a 2mm deep notch", and three specimens are conventionally tested at each temperature (TWI, impact testing). The same article warns that the results are qualitative: they are compared with a specification value and can't be used to calculate fracture toughness. Under D1.1, Charpy tests enter a PQR only when the contract documents call for them.

Key takeaway: no single destructive test qualifies a procedure, which is why a groove PQR pairs a strength test with a soundness test.

Worked example: the specimens from a 1 in. plate PQR

Inputs (illustrative). A fabricator qualifies a CJP groove weld procedure by test under AWS D1.1 on 1 in. plate. The base metal specification sets a minimum tensile strength of 65 ksi. The contract doesn't require Charpy tests. Specimen dimensions below are the measured values for this example; the code figures set the required shapes.

Step 1: non-destructive screening. The completed test plate is visually inspected and then radiographed or ultrasonically tested. It passes, so it is cut.

Step 2: specimen list. At 1 in., above the 3/8 in. boundary, the reported requirement is 2 reduced-section tension specimens and 4 side bend specimens: 6 specimens in all.

Step 3: tension tests.

SpecimenWidth (in.)Thickness (in.)Area (in.²)Maximum load (lbf)Tensile strengthFracture locationResult
T10.7501.0000.75052,40069,867 psi (69.9 ksi)Weld metalPass
T20.7480.9980.746550,90068,184 psi (68.2 ksi)Base metalPass

Area is width times thickness: 0.750 × 1.000 = 0.750 in.² and 0.748 × 0.998 = 0.7465 in.². Strength is load over area: 52,400 ÷ 0.750 = 69,867 psi and 50,900 ÷ 0.7465 = 68,184 psi. Both are above 65 ksi, by 7.5% and 4.9%. These are the same columns ASME's Form QW-483 uses: width, thickness, area, ultimate total load, ultimate unit stress, and type of failure and location.

Step 4: side bends. Each side bend specimen is a strip 3/8 in. thick, bent around a former 4 times that thickness in diameter, so 1.5 in. From bending geometry, the strain on the outer surface is about t ÷ (D + t) = 0.375 ÷ (1.5 + 0.375) = 0.20, or 20%. Every part of the weld, fusion line and heat-affected zone on that surface must stretch 20% without opening up.

SpecimenOpenings on the convex surfaceLargestSumResult against the reported limits (1/8 in. single, 3/8 in. sum)
S1Nonen/a0Pass
S2One, 1/16 in.1/16 in.1/16 in.Pass
S3Three: 3/32, 3/32 and 1/8 in.1/8 in.5/16 in.Pass (1/8 in. is not over 1/8 in.; 5/16 in. is under 3/8 in.)
S4One, 5/32 in., at the fusion line5/32 in.5/32 in.Fail (5/32 in. is over 1/8 in.)

The sum for S3 is 3/32 + 3/32 + 1/8 = 3/32 + 3/32 + 4/32 = 10/32 = 5/16 in. (0.3125 in.), under 3/8 in. (0.375 in.). S4's single opening of 5/32 in. (0.156 in.) exceeds 1/8 in. (0.125 in.).

Reading the result. The plate passed NDT and both tension tests, and still failed on one bend: a fusion-line flaw too tight to show before the test opened under 20% strain. The PQR can't be signed as it stands. The code's retest clause decides whether replacement specimens may be taken; if they also fail, the procedure is changed and a new plate is welded.

Key takeaway: 5 of 6 specimens passed and the procedure is still not qualified; qualification is all-or-nothing in a way production sampling is not.

Which tests do production welds need?

Production welds get non-destructive testing, and the extent comes from the code and the contract, not from the PQR. Passing a PQR doesn't reduce production inspection, and production NDT can't stand in for a missing PQR.

WorkWhat every production weld getsWhat is added by code or contract
Structural steel, AWS D1.1Visual inspection against the code's visual acceptance tableUT, RT, MT or PT where the contract documents call for it
Pressure vessels and piping, ASMEVisual examinationRT or UT at the extent the construction code sets (Section VIII, B31.3); Section IX sets none
Gas pipelines, 49 CFR Part 192Visual inspection by a qualified individual (192.241(a))NDT of a share of each day's field butt welds where 192.241(b) applies: at least 10% in Class 1 locations, 15% in Class 2 and 100% (at least 90% if impracticable) in Class 3 and 4 locations and within railroad or public highway rights-of-way (192.243(d))
Hazardous liquid pipelines, 49 CFR Part 195"Visual inspection must be supplemented by nondestructive testing" (195.228(a))At least 10% of each welder's girth welds each welding day, and all girth welds in listed locations, including railroad rights-of-way, subject to the rule's impracticability allowance (195.234(d) and (e))
Rail welds in trackVisual and alignment checks to the owner's standardUltrasonic testing where the owner's standard or AWS D15.2 is invoked

Our NDT welding inspection guide explains how each method works on a weld, and the comparison of non-destructive testing methods sets them side by side. For the structural acceptance rules, see AWS D1.1 weld inspection criteria and the AWS D1.1 visual inspection checklist.

Are production welds ever tested destructively? Rarely, because the test consumes the weld. Where it happens, it is by sampling: the gas pipeline rules let some welders keep their qualification by having "a production weld cut out, tested, and found acceptable" (192.229(d)(2)(i)), and a weld removed from service after an NDT rejection or a failure is often sectioned to find the cause.

Key takeaway: the PQR and the production NDT report are two different records, and an owner's file needs both.

How are welders tested?

A welder's qualification test judges the soundness of the deposit, not the strength of the joint, so it uses bends, break tests, macroetch or radiography, and no tension test. Strength was already proven by the PQR.

Study material for D1.1 says a groove welder's coupon is visually inspected first and then bend tested, and that radiography is permitted in place of the bends. Fillet welders are tested with a fillet break and a macroetch. Welder qualification is therefore the one place where codes commonly let an NDT method replace a destructive one.

The limits on that substitution are worth noticing. The gas pipeline rules say that "No welder or welding operator whose qualification is based on nondestructive testing may weld compressor station pipe and components" (49 CFR 192.229(a)). Procedure qualification has no such option under 192.225: the test welds are judged by destructive testing.

Where do thermite and flash-butt rail welds use destructive samples?

Rail weld programs use destructive samples at qualification: sample welds are made, then bent to failure, sectioned and hardness tested, before the process is used in track. Welds in track are then accepted by visual and ultrasonic inspection, because a rail weld can't be sampled without cutting it out.

AWS D15.2/D15.2M:2022, Specification for Joining Railroad Rail and Related Rail Components, is the AWS document for rail in track. AWS D1.1 covers structural steel and doesn't apply to it. The public preview of D15.2 shows where the destructive tests sit:

D15.2:2022 item (titles from the public preview)Test family
Clause 6.3, Slow Bend Testing and Acceptance for Thermite and Flash Welding Qualification; Table 6.8, Slow Bend Requirements; Figure 6.4, slow bend test configurationDestructive: bend to a required strength and deflection
Table 6.4, Post-Weld Chemistry Limits for Thermite Weld Metal; Figure 6.1, thermite fusion zone for chemistry sample and hardness testingDestructive: chemical analysis and hardness on a sectioned weld
Figure 6.2, Location and Spacing of FW Hardness Indents; Figure 6.3, FW Macroetch Test SampleDestructive: hardness traverse and macroetch of a flash weld
Tables 6.6 and 6.7, Testing Requirements for TW and FW QualificationThe list of qualification tests
Table 8.1, Visual Inspection; Table 8.2, Ultrasonic Inspection Acceptance Requirements; clause 8.4, Verification of Non-Destructive Testing (NDT) ResultsNon-destructive: acceptance of production welds

The requirements inside those clauses are paywalled and aren't reproduced here. AREMA's Manual for Railway Engineering, Chapter 4, Part 3, lists two recommended-practice specifications by title in its 2025 table of contents: 3.10, Specification for the Quality Assurance of Electric-Flash Butt Welding of Rail, and 3.13, Specification for the Quality Assurance of Thermite Welding of Rail. Whether a welding plant also breaks periodic sample welds during production is set by the quality assurance specification the owner adopts.

What the slow bend test does. A welded rail is loaded in four-point bending until it breaks, and the modulus of rupture and the deflection are recorded. A 2013 Transportation Technology Center (TTCI) digest explains the orientation and the trade-off:

"The 4-point slow bend test places the base of the weld in tension. Because the capability of materials to deflect under bending loads generally decreases as hardness increases, welds with harder bases tend to fail at lower deflections." (TTCI Technology Digest TD-13-029)

A published case where NDT and destructive results differed. In a 2019 TTCI digest on high-hardness thermite welds in 136RE rail, all the welds were tested with 0-degree, 45-degree and 70-degree ultrasonic probes and no flaw indications were found. Four welds then went to slow bend tests against the AREMA values the digest cites for rail over 341 BHN (120,000 psi modulus of rupture and 0.60 in. deflection). Three passed. Of the first two, the digest says "the second weld failed to qualify the minimum limit for deflection even though the modulus of rupture limit was reached" (TTCI Technology Digest TD-19-010). The ultrasonic test was clean and correct: there was no flaw to find. Ductility is a property, and only a destructive test measures it. Treat the two figures as historical; take current values from the edition your contract cites.

Qualification programs mix both families. A 2006 TTCI digest lists the laboratory regime for a robotic gas metal arc rail head repair weld as "rolling load, slow bend, Charpy impact, tensile, longitudinal, and transverse hardness testing, micro- and macro-examination, radiography, and ultrasonic testing" (TTCI Technology Digest TD-06-008).

What FRA requires. 49 CFR Part 213 sets no weld qualification test. A search of the 2025 text of Part 213 finds no use of "destructive", "slow bend", "bend test", "procedure qualification" or "welder". What Part 213 regulates is the weld in service: 213.113(d)(6) defines a defective weld by discontinuities "exceeding 5 percent of the rail head area individually or 10 percent in the aggregate", and those are found by internal rail inspection, which is non-destructive. Our guide to rail weld inspection covers the in-track side, with detail in aluminothermic weld inspection and flash butt weld inspection.

Key takeaway: for rail welds, destructive tests qualify the kit, the machine settings and the welder; ultrasonic and visual inspection accept the weld in track.

Which test answers which question?

Match the test to the question being asked, then to the code that asks it.

QuestionTestFamilyWhere it normally appears
Is the joint as strong as the base metal?Reduced-section tensionDestructiveGroove-weld PQR
Is the weld sound and ductile through the thickness?Guided bend (root, face or side)DestructiveGroove-weld PQR; welder qualification
Did the weld fuse to the root, and is the size there?MacroetchDestructiveFillet and partial-penetration PQR; flash-butt rail weld qualification
What does the inside of the weld look like?Nick-break; fillet breakDestructivePipeline qualification; fillet welder qualification
Is any zone too hard?Hardness (Brinell on bulk areas, Vickers traverse across a weld)Destructive when made on a cut sectionRail weld qualification; PQRs when the contract requires it
Will the joint resist brittle fracture at low temperature?Charpy V-notchDestructivePQRs when toughness is specified
Does a welded rail have the bending strength and ductility for track?Slow bendDestructiveThermite and flash-butt qualification
Are there surface defects on this weld?VT, then MT or PTNon-destructiveEvery production weld (VT); others by contract
Are there internal defects in this weld?UT or RTNon-destructiveProduction welds at the extent the code or contract sets; D1.1 test plates before cutting

What do specifications get wrong about weld testing?

Most errors come from asking one family of test to do the other's job.

  1. "100% UT in lieu of procedure qualification." Production NDT can't supply tensile strength, ductility or toughness. A procedure is prequalified, qualified by test, or not usable.
  2. Requiring bend and tension tests for every D1.1 procedure. A prequalified WPS inside the Clause 5 limits needs no PQR.
  3. Calling for Charpy tests without a temperature and an energy. A toughness requirement needs both numbers and the notch locations, and it adds supplementary variables to the procedure.
  4. Citing AWS D1.1 or D15.1 for rail welds. D1.1 is the structural steel code and D15.1 covers railcars and locomotives. Rail in track is AWS D15.2 with the owner's standard.
  5. Assuming a welder's radiographed coupon qualifies the procedure. Radiography can stand in for bends in welder qualification where the code allows; it doesn't qualify a WPS.
  6. Leaving the edition out. "Slow bend per AREMA" or "bends per D1.1" without a year invites the wrong limits.

What destructive and non-destructive testing can't tell you

Each family has a blind side, and it is the other family's strength.

  • A PQR is one weld. It shows the procedure can work, not that every production weld did.
  • Destructive specimens are small samples. A bend specimen tests the strip it was cut from. A defect elsewhere in the test plate is missed unless NDT screened the plate first.
  • NDT measures no mechanical property. A weld with no indications can still be too hard, too brittle or understrength if the procedure was wrong.
  • NDT has its own detection limits. Tight or poorly oriented planar flaws can be missed by RT and UT alike; see our page on lack of fusion in welds.
  • Neither family replaces process control. Fit-up, preheat, consumable handling and, for thermite welds, the kit maker's procedure decide weld quality before any test is made.

Key takeaway: specify both families, each for the job it can do, and name the code edition for each.

How EMA Industries applies this

EMA Industries provides weld examination, including AWS D1.1 structural weld UT, magnetic particle testing and liquid penetrant testing, rail weld inspection, WPS and PQR support, and NDT Level III technical support. The company supports work in Southern California and mobilizes for projects throughout the United States. The destructive tests described here are laboratory work arranged by the organization qualifying the procedure; EMA's part is the non-destructive side, on the qualification test plate where the code calls for it and on production welds. For weld UT, MT and PT scopes, see ultrasonic examination services or contact EMA Industries.

Frequently asked questions

What is destructive weld testing?

Destructive weld testing is mechanical testing of specimens cut from a test weld: tension, guided bend, macroetch, nick-break, hardness and Charpy impact tests. The specimens are pulled, bent, broken or sectioned, so the test weld is consumed. It is used to qualify welding procedures and welders, not to accept production welds.

Which destructive tests does a PQR require under AWS D1.1?

For a complete-joint-penetration groove weld, public study references report two reduced-section tension specimens and four bend specimens: two root and two face bends for plate 3/8 in. and thinner, and four side bends for thicker plate. The test plate is visually inspected and tested by RT or UT before cutting. Charpy tests are added only when the contract documents require them. Confirm the counts in your edition.

Can NDT replace destructive testing for procedure qualification?

Not for the mechanical properties. Radiography and ultrasonic testing find discontinuities, but they can't measure tensile strength, ductility or toughness, which is what a PQR records. The federal pipeline rule is explicit that procedure test welds "must be determined by destructive testing". Welder qualification is different: some codes allow radiography in place of bend tests there.

Are production welds destructively tested?

Production welds are normally accepted by visual inspection and NDT, because a destructive test consumes the weld. Exceptions are sampling arrangements written into a code or contract, such as cutting out a production weld to maintain a pipeline welder's qualification under 49 CFR 192.229, and sectioning a rejected or failed weld to find the cause.

What is a slow bend test on a rail weld?

A slow bend test loads a welded rail in four-point bending, with the base of the weld in tension, until it breaks. The modulus of rupture and the deflection are compared with minimums in the owner's specification, AWS D15.2 or AREMA recommended practice. It is a qualification test for thermite and flash-butt welding, not a test applied to welds in track.

Sources

← All articles