Ultrasonic rail testing for metro and light rail systems sends 70° and 0° beams into the running rail, usually from a walking-speed cart, to find internal flaws. Most urban transit track is outside FRA's Part 213 under 49 CFR 213.3(b)(3), so test intervals and defect rules come from the agency's standards under FTA state safety oversight (Part 674).
This article covers the technical side of transit testing: embedded and girder rail, grooved profiles, third rail and traction power, tight curves, short night possessions, and how cart and hand testing compare. For national freight and short-line testing, see ultrasonic rail testing services in the USA. For procurement, RFPs and jurisdiction in detail, see rail inspection services for government and transit authorities.
Who regulates ultrasonic rail testing for metro and light rail systems?
For most urban rail transit, the agency and its state safety oversight agency (SSOA) set the testing rules, not FRA. FRA's track standards exclude isolated rapid transit. Section 213.3(b)(3) says Part 213 does not apply to:
"track used exclusively for rapid transit operations in an urban area that are not connected to the general railroad system of transportation." — 49 CFR 213.3(b)(3)
Federal oversight of that track comes through the FTA. Under 49 CFR Part 674, each state's SSOA must adopt a program standard that explains how it develops and adopts "minimum standards for safety" and includes a risk-based inspection program (674.27(a)(2) and (a)(12)). Part 674 sets no rail flaw test interval and never mentions ultrasonic testing (2025 CFR text search). The interval, the defect table and the remedial actions are written into the agency's own track maintenance standard. In California the SSOA is the CPUC, whose rail transit rules include General Order 143-B (light-rail safety) and GO 164-F (state safety oversight).
| Where the track sits | Whose testing rules apply |
|---|---|
| Isolated subway, elevated or light rail, not connected to the general system | The agency's track standard, overseen by the SSOA (FTA Part 674); CPUC in California |
| Transit track connected to, or shared with, the general railroad system | FRA Part 213 applies, including the 213.237 internal rail test intervals |
| Commuter rail on the general system | FRA Part 213 |
Where FRA does apply, 49 CFR 213.237 sets the internal test interval by track class and tonnage. Jurisdiction questions for shared corridors and contracts are covered in the government and transit authorities article.
Key takeaway: check which rulebook governs each segment before you write a test scope, because a mixed system can have both.
Which standards describe how to test rail in track?
For rail in track, EN 16729-1 and ISO 5735-1 are the in-track ultrasonic testing standards. ISO 17640 is a weld standard and doesn't cover rail flaw detection. No US federal rule prescribes an ultrasonic method. Part 213 has no beam angles, no calibration method and no test speed. It only requires that the equipment performs "as intended" and can test between joint bars.
| Reference | What it covers | Use on a transit system |
|---|---|---|
| EN 16729-1:2016 | Ultrasonic testing of rails installed in track, by dedicated test vehicles or manually propelled devices, to give comparable results on flaw location, type and size | A useful technical reference. Its scope says it "applies only to rail profiles meeting the requirements of EN 13674-1", the flat-bottom rail standard, so grooved rail is outside it. A revision (prEN 16729-1) was in development in 2026 |
| ISO 5735-1:2024 | The same subject at ISO level; applies only to flat-bottom (Vignole) rail of 43 kg/m and above, and "treats welded joints as plain rail" | Same limits as EN 16729-1; no grooved rail |
| AREMA Manual for Railway Engineering, Chapter 4 (Rail) and Chapter 12 (Rail Transit) | Recommended practice, not regulation. AREMA Committee 4 has a subcommittee on rail NDT. The 2024 Chapter 12 table of contents lists an Embedded Track part, while its Maintenance of Way part is marked "Reserved" | Check the current edition for any rail testing guidance before citing a clause; the MRE is paywalled |
| 49 CFR 213.237, 213.238, 213.113 | FRA intervals, operator qualification and remedial actions | Mandatory only on track under FRA; widely borrowed as a template by transit standards |
| ISO 17640 | Ultrasonic testing of welded joints (techniques, testing levels, assessment) | Not a rail flaw detection standard. The original article cited it in error |
Key takeaway: name the reference your agency's standard adopts, and write grooved-rail calibration into the procedure yourself, because neither in-track standard covers it.
What makes transit track harder to test than freight track?
Five conditions that are rare on freight lines cause most of the difficulty on transit track: embedded rail, grooved profiles, traction power, tight curves and short possessions. Each one reduces coverage, slows the test or both.
| Condition | Effect on ultrasonic testing | Usual response |
|---|---|---|
| Embedded and girder rail in street running | Only the running surface is reachable; web and base are buried | Head-only search plus a written statement of what wasn't tested |
| Grooved rail profiles | Debris and water in the groove; guiding lip beside the head; no in-track standard | Clean the groove first; calibrate on a reference rail of the same section |
| Third rail or overhead power | Work only under the agency's power and roadway worker protection rules | Power status in the briefing; agency verifies power removal |
| Tight curves | Gauge-corner RCF and wear on the high rail mask or misalign the beam | Gauge-corner probes, hand follow-up, grinding before retest |
| Short possession windows | Testing time is a fraction of the window | Plan by effective test hours, not clock hours |
Embedded and girder rail in street running
Street-running light rail sits in concrete or asphalt with only the railhead exposed. One design guideline for light rail circulators puts it plainly: track embedded in concrete "is not very maintenance-friendly. Access is only by jackhammer" (Graebner, Jackson and Lovejoy, Trackway Infrastructure Guidelines for Light Rail Circulator Systems, April 2007).
That has three effects on ultrasonic testing. First, the probe can only sit on the running surface, so the rail base can't be checked by hand from the foot or the web side, as it would be at a thermite weld on open track. Second, many embedded rails sit in an elastomer boot for stray-current insulation, which keeps the web and base out of reach. Third, the street is not a closed site. Road traffic, pedestrians and paving debris all affect the work, and the groove fills with grit, water and de-icing residue that break the couplant film under the probe.
Expect lower test speeds on embedded track, more stops to re-establish coupling, and a test record that lists every length where coupling was lost. Untested rail is untested rail, not a false call.
Grooved rail profiles
Grooved rail (also called girder rail) carries a flangeway groove in the head, with a lip on the gauge side. European grooved sections are made to EN 14811:2019, which covers grooved rails of 42 kg/m and upwards for tram systems; 59R2 (also known as Ri59N) is a common profile. The 2007 circulator guideline notes that there are no North American producers of girder rail, so US systems that use grooved rail mostly buy European sections.
For the ultrasonic test, the grooved head is narrower and asymmetric. Side-looking and gauge-corner probes must clear the lip. Neither EN 16729-1 nor ISO 5735-1 covers grooved profiles, so the reference blocks, probe positions and sensitivity settings have to be set on a reference piece of the same section. One manufacturer of a grooved-rail test trolley states that its scan covers the whole rail section "except for the foot flanges and the checkrail" (vendor brochure, UDS2-77 SC). Treat that as typical: a cart searches the head and web, not the base flanges or a guard lip.
Third rail, overhead power and de-energization
Heavy rail metros usually run on third rail, and light rail on overhead contact wire. Either way, the testing crew works inside the agency's roadway worker protection program under 49 CFR Part 671, FTA's rail transit roadway worker protection rule. Part 671 doesn't apply to rail systems under FRA safety oversight (671.1(b)), and FRA's own Part 214 has no third-rail provision at all.
Under 671.33(b)(3), for agencies with electrified systems the job briefing "must include the status of power and hazards explicitly related to the electrified system". Among the redundant protections listed in 671.39(d)(2)(x) is restricting work to times when "propulsion power is down with verification that track is out of service". Training under 671.41 must cover traction power hazards where they apply.
In practice, the agency removes and verifies power, not the testing contractor. The test plan should state who does this, when the crew may foul the track, and how power restoration is confirmed at the end of the window. Ask also whether the test cart's wheels are electrically insulated, because a cart that bridges the two running rails can show as an occupied track circuit. That is good practice to confirm with the agency's signal department, not a rule.
Tight curves and gauge-corner RCF masking
Curves on transit systems are far sharper than on freight lines. A 2007 guideline describes 25 m (82 ft) as the de facto minimum curve radius for US light rail, and lists legacy systems below it, down to 10.8 m (35.4 ft) in Philadelphia. On curves that tight, the high rail develops rolling contact fatigue at the gauge corner: head checks, then shelling and spalling.
That damage hurts ultrasonic testing in two ways. Shells and surface cracks reflect or scatter the beam before it reaches the head, and detail fractures start from exactly that damage, so the defect most likely to grow is the one best hidden. Gauge-side wear also tilts the contact surface, so a fixed-angle probe searches the wrong volume of steel. The data back this up:
- In a TTCI test on rails with drilled reflectors, average relative 70° response on the gauge side was 68%, against 80% on the field side (TD-18-027).
- The NTSB noted that a lower gauge-corner fatigue crack is "not easily scanned by ultrasonic equipment" (RAB-16/01).
- FRA's handheld UT study found that flat probes couple poorly on heavy gauge-face wear (DOT/FRA/ORD-26/07, 2026).
Corrective grinding helps. TTCI research found that grinding restored a valid test at 77% of 88 exceptions, and at all of them where at least 0.060 in. was removed. The order matters on curves: grind, then test, then follow up suspect gauge-corner indications by hand.
Short possession windows
Transit testing happens in the gap between the last and first revenue trains, often only a few hours on weeknights. From that window, subtract the power-down and verification, the roadway worker briefing, travel to the start point, calibration checks at both ends and the clear-up. What's left is often 2 hours or a little more of actual testing. The worked example below plans a whole system on that basis. Tunnel sections add lighting, ventilation and walkway limits on top of this.
How do cart and manual ultrasonic testing compare on transit track?
A walking-speed cart (trolley) gives continuous, recorded coverage of the head and web; a hand probe gives targeted coverage where the cart can't reach. Most transit programs use both. The table below describes typical practice, not a standard, and the detection points come from freight research because no published study compares transit carts and hand probes directly.
| Factor | Walking-speed cart (trolley) | Manual hand probe |
|---|---|---|
| Typical beams | Several fixed probes: 0°, 70°, and about 37–45° or side-looking | One probe at a time, angle chosen for the target |
| Speed | One grooved-rail trolley lists up to 5 km/h (3.1 mph); stop-and-verify lowers the average | Feet per minute, not miles per hour |
| Coverage | Head and web of the running rail in one pass; not the base flanges, check rail or guard lip | Wherever the probe can be placed: weld base on open track, switch points, frog-area rail, verification of cart suspects |
| Record | Encoded B-scan and A-scans tied to position | A-scan readings and a written record unless the unit stores data |
| Repeatability | Fixed probe positions, but the operator still sets calibration | Depends heavily on the operator. ORD-26/07 found that, with a small exception, no two operators produced statistically similar calibrations |
| Best use on transit | Plain track in short windows, including embedded head-only search | Thermite weld bases on open track, special trackwork, gauge-corner sizing, retests |
| Main weakness | Loss of coupling on corrugated, contaminated or worn rail | Slow; coverage gaps if scanning isn't systematic |
For context, an FRA-sponsored trial of six hi-rail systems in 1999 found 72% of 49 known defects overall and only 33% of bolt hole cracks (TTCI TD-99-006). Field welds need hand UT of the base, because test cars miss most of it (TTCI TD-00-013). Those are freight vehicle figures, so use them only as a reminder that no single method covers the whole rail. For more on cart equipment, see ultrasonic rail detection carts and manual vs automated ultrasonic testing.
Which defects does ultrasonic testing find, and what are they called?
Ultrasonic testing finds internal rail defects, and the 49 CFR 213.113(d) defect names are the common vocabulary for them, even on systems outside FRA. Each agency adopts its own defect table and remedial actions in its track standard. Many base theirs on 213.113, but the size bands and speed limits can differ, so report using the agency's table.
| 213.113 term | Where it starts | Sized by | Typical UT beam |
|---|---|---|---|
| Transverse fissure | Inside the head, from a crystalline center or nucleus | % of head cross-section | 70° |
| Detail fracture | At or near the head surface, from shelling, head checks or flaking | % of head cross-section | 70°; often masked by the shells it grows from |
| Compound fissure | Starts as a horizontal split head that turns up or down | % of head cross-section | 0° and 70° |
| Engine burn fracture | Where driving wheels slipped on the rail | % of head cross-section | 70° |
| Defective weld | In a field or plant weld (lack of fusion, slag, porosity, cracking) | % of head (transverse) or length (longitudinal) | 70° and 0°; base by hand probe |
| Horizontal split head | In the head, usually at least 1/4 in. below the running surface | Length | 0° (loss of back-wall echo) |
| Vertical split head | Vertical split through or near the middle of the head | Length | 0° and side-looking probes |
| Head and web separation, split web | Fillet between head and web; web | Length | 0° and 37–45° |
| Bolt hole crack | From a bolt hole at a joint | Length | 37–45° |
| Broken base | In the base flange | Length | Hand probe and visual; carts largely miss the base |
Part 213 sizes the head defects by percentage of head area. For example, on FRA track a transverse fissure of 5 to under 25% of the head takes remedial action C, which means joint bars within 10 days. An agency's table may set different bands. Corrugation, which is common on transit curves, is not a 213.113 defect at all: the definition of flattened rail excludes it. See corrugation on rail and FRA defect codes explained.
Worked example: how many nights does a 20-mile light-rail system take?
A 20-mile double-track light-rail system needs about 27 nights for one cart crew working alone, or about 18 nights with a second crew testing turnouts in parallel, under the assumptions below. The numbers are illustrative. Use your own window, track mix and test rates.
Inputs (assumed):
- 20 route-miles of double track = 40 track-miles: 34 track-miles of ballasted or direct-fixation track and 6 track-miles of embedded street track (3 route-miles)
- 40 mainline turnouts, tested by hand
- Window: last train clears at 1:15 a.m., first train at 4:45 a.m. = 210 minutes
- One cart that tests both rails of a track in one pass (or two single-rail units side by side)
Step 1: effective test time per night
| Activity | Minutes |
|---|---|
| Possession window | 210 |
| Power-down, verification, roadway worker briefing, working limits | −30 |
| Travel to start, set-up, start-of-shift calibration check | −25 |
| End-of-shift calibration check, clear track, restore power | −25 |
| Effective test time | 130 (2.17 h) |
Step 2: nights per track type
| Work | Assumed rate | Per night | Quantity | Nights |
|---|---|---|---|---|
| Open track (cart) | 1.5 mph average with stop-and-verify | 2.17 h × 1.5 = 3.25 track-miles | 34 track-miles | 34 ÷ 3.25 = 10.5 → 11 |
| Embedded track (cart) | 0.75 mph (groove cleaning, coupling stops) | 2.17 h × 0.75 = 1.63 track-miles | 6 track-miles | 6 ÷ 1.63 = 3.7 → 4 |
| Turnouts (hand) | 25 minutes each | 130 ÷ 25 = 5.2 → 5 turnouts | 40 turnouts | 40 ÷ 5 = 8 |
| Subtotal, one crew | 23 | |||
| Contingency for cancelled windows and retests (15%) | 23 × 1.15 = 26.5 → 27 |
Step 3: with a second crew. If a hand-testing crew does the turnouts on the same nights, the cart's 15 nights (11 + 4) set the length: 15 × 1.15 = 17.3 → 18 nights.
Two more checks are worth making. Couplant: one grooved-rail trolley maker quotes about 1 liter of water per kilometer per rail. At 3.25 track-miles (5.23 km) a night on two rails, that's about 10.5 liters a night. Retests: if 5% of the open track (1.7 track-miles) loses coupling and must be retested, that's about half a night, which the 15% contingency covers. Weekend or extended possessions shorten the program sharply, because the fixed 80 minutes of set-up and clear-up are spread over more test time.
What should a transit rail test record show?
The test record should show what was searched, what wasn't, and what was found, segment by segment. On FRA track, 213.241 lists the required content. On transit track the agency's standard sets it, but the same items make the record defensible:
- Line, track, direction, and the start and end stationing or mileposts of each run
- Rail type for each length (T-rail or grooved section, embedded or open)
- Every length not validly searched, with the reason (coupling loss, debris, grinding needed, possession ended)
- Each indication: location, rail (left or right), defect type in the agency's terms, size, and the action the agency's table calls for
- Possession log: window start and end, power-down and restoration times
- Equipment, probe set, calibration checks, and the operator's qualification
Deliverables, scoring and contract terms belong in the procurement scope. See the government and transit authorities article for those, and how often rail must be tested for interval planning.
What can't ultrasonic testing find on transit track?
Ultrasonic rail testing searches the running rail's head and web well. It searches the base, guard lips and cast special trackwork poorly or not at all. The main limits on transit systems are:
- Rail base in embedded track. With the base in concrete or a boot, neither a cart nor a hand probe can reach it. Base cracks and corrosion there go unseen until the rail breaks or the track is excavated.
- Check rails and grooved-rail guard lips. Test trolleys typically leave them out of the scan.
- Defects under shells and head checks. Surface damage masks detail fractures, mainly on the high rail of tight curves. Grinding before testing improves coverage.
- Cast manganese frogs. The coarse grain of austenitic manganese steel scatters sound. FRA research reports that in-service examination of these castings uses visual inspection only (FRA RR 22-25). See turnout inspection.
- Corrugated and contaminated rail. Corrugation and street debris break coupling. The result is untested rail, which must be recorded and retested.
- Weak or closed cracks. Tight, compressed cracks transmit sound and reflect little, so small flaws can pass between tests.
- Grooved rail calibration. Neither EN 16729-1 nor ISO 5735-1 covers grooved profiles, so detection settings rest on the agency's or contractor's own procedure.
A test also gives no information about the third rail or overhead contact system, insulated joints' electrical condition, or track geometry. Those need their own inspections.
How EMA Industries applies this
EMA Industries performs ultrasonic rail flaw testing for transit agencies, short lines and industrial track owners. We're based in Southern California and mobilize nationwide. On a transit system, the test plan should start from the agency's own track standard and possession calendar, list embedded and grooved sections separately, and report every untested length. To scope a transit testing program, see our ultrasonic rail testing services or contact us.
Related reading: Ultrasonic rail testing services in the USA · Rail inspection for government and transit authorities · Tunnel rail inspection · Rail shelling and spalling
Frequently asked questions
How often is light rail track tested ultrasonically?
The interval comes from the agency's own track standard unless the track is under FRA. No federal rule sets a fixed interval for isolated transit track, and FRA's 213.237 intervals are often used as a model. On track under FRA, 213.237 applies by class and tonnage.
Can a test cart inspect embedded street track?
A cart can search the head and web of embedded rail from the running surface if the groove is clean and coupling holds. It can't reach the base, which is buried in concrete or a rail boot. Lengths where coupling is lost must be recorded and retested.
Why do tight curves cause missed defects?
The high rail on a tight curve develops head checks and shelling at the gauge corner. That surface damage scatters the beam and hides detail fractures that grow from it, and gauge wear misaligns fixed-angle probes. Grinding before testing and hand follow-up on gauge-corner suspects reduce the risk.
Who turns off the third rail before testing?
The transit agency removes and verifies traction power under its roadway worker protection program, not the testing contractor. Under 49 CFR 671.33(b)(3), the job briefing on an electrified system must include the status of power. The test plan should name who removes, verifies and restores power.
Is ISO 17640 a rail testing standard?
ISO 17640 covers ultrasonic testing of welded joints, not rail flaw detection in track. The in-track references are EN 16729-1 and ISO 5735-1, both limited to flat-bottom rail, plus the agency's standard and, where FRA applies, 213.237.
Sources
- 49 CFR 213.3, Application, eCFR; read on Cornell LII, October 2026
- 49 CFR 213.113, Defective rails, eCFR
- 49 CFR 213.237, Inspection of rail, eCFR
- 49 CFR Part 674, State Safety Oversight, eCFR; 674.27 read on Cornell LII
- 49 CFR Part 671, Rail Transit Roadway Worker Protection, eCFR; 2025 CFR text on govinfo
- CPUC rail transit rules and regulations (GO 143-B, GO 164-F, GO 175-A)
- EN 16729-1:2016, Non-destructive testing on rails in track, Part 1, standard listing and scope
- ISO 5735-1:2024, Non-destructive testing on rails in track, Part 1, BSI listing; scope from genorma
- EN 14811:2019, Grooved rails and associated construction profiles, BSI listing
- AREMA Manual for Railway Engineering, store page; Chapter 12 (Rail Transit) table of contents, 2024
- Graebner, Jackson and Lovejoy, Trackway Infrastructure Guidelines for Light Rail Circulator Systems, April 2007 (hosted by NACTO)
- TCRP Report 155, Track Design Handbook for Light Rail Transit, 2nd ed., 2012; 3rd edition project record on TRID
- Bruzek, Einbinder and Tunna, MAPOD for Handheld Rail Ultrasonic Testing, DOT/FRA/ORD-26/07, July 2026, ROSA P
- Wilson and Poudel, FRA RR 22-25 (special trackwork UT feasibility), 2022, ROSA P
- TTCI Technology Digests TD-99-006 (1999), TD-00-013 (2000) and TD-18-027 (2018), MxV Rail
- NTSB Railroad Accident Brief RAB-16/01 (Lynchburg, 2014), NTSB
- UDS2-77 SC grooved-rail trolley brochure (manufacturer, vendor claims), ndt.com.ua